--- dombaines <dombaines@...> wrote: > So what is in a simple tin salt mix... The Metal Finishing Guidebook lists three formulations for immersion deposits of tin onto copper, only one formula is cyanide-free. Here is that formula: Stannous chloride 3.8 g/L Thiourea 49.5 g/L Sulfuric acid 12 ml/L Combine the compounds at a temperature of 80-120 degrees Fahrenheit. The crystals in TINNIT and other similar products are of a similar chemistry (But, in solid crystal form). There is simply no other way to do it without using cyanide salts. Best regards Marvin Dickens Alpharetta, Georgia USA ===== Registered Linux User No. 80253 If you use linux, get counted at: http://www.linuxcounter.org __________________________________ Do you Yahoo!? Protect your identity with Yahoo! Mail AddressGuard http://antispam.yahoo.com/whatsnewfree
Message
Re: [Homebrew_PCBs] Re: Tin salts
2003-11-13 by mpdickens
Attachments
- No local attachments were found for this message.