--- In Homebrew_PCBs@yahoogroups.com, Leon Heller <leon355@...> wrote: > > On 26/11/2011 18:00, DaveC wrote: > > >... > > >HCl/H2O2 is very fast anyway, but it could probably be useful for CuCl2. > > > > > >Leon > > > > -=-=-=- > > > > I found it not so fast. I etched a 5" x 10" 1-sided board (consisting > > of several duplicate small circuits) and it took almost an hour. I > > started with a fresh batch, just enough etchant to cover the board > > but added more as time dragged on. > > > > Maybe my mix is wrong? I'm using 15 percent hcl (muriatic acid) and 3 > > percent h2o2 at a mix of 1:1. > > > > What mix are you using? > > It was a long time ago, I can't remember. IT would have been 30% HCl, > because that is what I have available. It only took about 30 seconds, > though. > > Leon > -- > Leon Heller > G1HSM > Could be 15% HCl is too low, and maybe you should have a 1:2 ratio My HCl says "383g/litre" - would that mean 38%?