"awakephd" <a_wake@...> writes: > I am following up on a comment in an earlier thread, to the effect > that starting with 2 parts drug store hydrogen peroxide + 1 part > Muriatic acid, one cannot ever get to the point of having CuCl2. This is wrong - I did exactly that. I started with two parts 3% (drugstore) peroxide and one part 37% (hardware store) HCl, added copper, and now have a tank of gleaming green CuCl etchant. It's not instant - I dumped the copper in the tank, turned on the air bubbler, and waited - it took a few days to completely convert (3 liters solution, 0.5 lb copper). Probably would have gone faster if I had put the copper in right away, but I didn't figure that part out until a few days had past, and most of the H2O2 was decomposed, so I had to pour more in.